Phase Diagrams and Solidification

Phases and microconstituents, binary diagrams, the Gibbs phase rule and the lever rule, eutectic systems, precipitation, the invariant reactions, intermetallic compounds, the Fe-C system with the microstructures of steels, and ceramic and ternary diagrams.

📖 Source: Universidad Carlos III de Madrid · Session 7 T4 Phase diagrams I_2025.pdf, Session 8 T4 Phase diagrams II.pdf, Session 9 T4 Phase diagrams III.pdf and Session 10 T4 Phase diagrams IV.pdf

Central idea: a phase diagram is a map that tells which phases are stable in a material for each temperature, pressure and composition. Reading it gives three answers for any alloy at any temperature: which phases are present, what each phase is made of, and how much of each there is.

This page follows the official slides of Topic 4 in order. Part I (Session 7) covers the basic vocabulary, one-component diagrams, binary isomorphous systems, the Gibbs phase rule, the tie line and the lever rule, non-equilibrium solidification and binary eutectic systems. Part II (Session 8) covers solid-state precipitation, the invariant reactions, intermetallic compounds and congruent and incongruent melting. Part III (Session 9) covers the Fe-C system, the equilibrium transformations of steels and the influence of alloying elements. Part IV (Session 10) covers ceramic and ternary phase diagrams. Worked examples use only data printed on the slides.

Part I — Phase diagrams I (Session 7)

§ 1 Component, phase and microconstituent [Session 7 Slide 2]

Three words are used all through the topic, and they mean different things:

The slide illustrates the three words with food: the components of a potato are water, protein, fat, carbohydrates and so on (a table of grams per 100 g); the potato itself plays the role of a phase; and fries, a structure you can see and that is made from the potato, play the role of a microconstituent.

In a real material, the micrograph below shows a steel with two microconstituents. Region 1 is ferrite, a single phase. Regions 2 and 3 are pearlite, a microconstituent made of two phases (ferrite and cementite) arranged in thin alternating plates.

Micrograph of a steel with ferrite and pearlite
Figure 1. Microconstituents in a steel: 1 is ferrite, 2 and 3 are pearlite (ferrite + cementite). From Session 7 Slide 2.

§ 2 The equilibrium phase diagram [Session 7 Slide 3]

An equilibrium phase diagram (also called a stability map) is a map of the phases in thermodynamic equilibrium that are present in a system of materials at different pressures, temperatures and compositions.

The slide uses the phase diagram of CO₂ as an example:

Phase diagram of CO2
Figure 2. Phase diagram of CO2 (labels in Spanish: Sólido, Líquido, Gas; Presión, Temperatura): triple point at 5.1 atm and −56.6 °C, sublimation at 1 atm and −78.2 °C, critical point at 73 atm and 31.1 °C. Copied from Session 7 Slide 3.
Worked example 1 — Why dry ice does not melt at 1 atm

Question. A block of solid CO₂ is heated at a constant pressure of 1 atm. What phases appear?

Reading the diagram. Follow the horizontal line $P$ = 1 atm from left to right. Since 1 atm is below the pressure of the triple point (5.1 atm), the line never enters the liquid region: it goes from the solid region straight into the gas region, crossing the sublimation line at −78.2 °C.

Answer. The solid turns directly into gas at −78.2 °C (sublimation). Liquid CO₂ can exist only at pressures above 5.1 atm, which is why there is no liquid CO₂ at room conditions [Session 7 Slide 3].

§ 3 Unary (one-component) diagrams [Session 7 Slides 5-6]

With a single component the composition is fixed, so the diagram is drawn with pressure and temperature as axes (a P-T diagram).

3.1 Water [Session 7 Slide 5]

The P-T diagram of water has three lines that meet at the triple point $P_T$: the sublimation line (A to $P_T$), the melting line ($P_T$ to B) and the vaporisation line ($P_T$ to C). Cooling at constant pressure along the dashed line, the water vapour first crosses the vaporisation line at $T_v$ and then the melting line at $T_m$.

Phase diagram and cooling curve of water
Figure 3. Left: P-T diagram of water with the sublimation (A to P_T), melting (P_T to B) and vaporisation (P_T to C) lines and the triple point P_T; the dashed line is the cooling path at constant pressure. Right: its cooling curve, with the plateaus 2 (condensation at T_v) and 4 (solidification at T_m). The blue marks are handwritten on the slide. Copied from Session 7 Slide 5.

The cooling curve on the right records the temperature against time along that path. In the stretches 1, 3 and 5 a single phase cools down. In the plateaus 2 (condensation at $T_v$) and 4 (solidification at $T_m$) the temperature stays constant while two phases coexist, because the heat released by the transformation compensates the heat that is lost.

On a diagram with pressure on a log scale, the vertical line at 1 atm meets the melting line at 0 °C (water/ice) and the vaporisation line at 100 °C (steam/water):

Water at 1 atm on a log-pressure diagram
Figure 4. Temperature against pressure (log scale) for water: at 1 atm the vertical line meets the melting line at 0 °C and the vaporisation line at 100 °C. Copied from Session 7 Slide 5.

At very high pressures (up to several GPa) water has many different solid phases, the different crystal structures of ice:

Phase diagram of water up to 4 GPa
Figure 5. Water at high pressure (up to 4 GPa): several crystal structures of ice (I, II, III, V, VI, VII, VIII), each a different solid phase. From Session 7 Slide 5.

3.2 Pure iron [Session 7 Slide 6]

Solid iron has three different crystal structures, each a different phase: α-Fe (BCC) below 910 °C, γ-Fe (FCC) between 910 and 1394 °C, and δ-Fe (BCC) from 1394 °C up to the melting point, 1538 °C. Different phases coexist at the triple points. The slide compares the three solid structures with three varieties of potato (yellow, red and purple) and the liquid with potato purée: the same "substance" in different forms.

Phase diagram of pure iron
Figure 6. P-T diagram of pure iron (pressure on a log scale) with α-Fe (BCC), γ-Fe (FCC), δ-Fe (BCC), liquid and vapour, the triple points and the slide's potato analogy. Copied from Session 7 Slide 6.

§ 4 Binary isomorphous diagrams [Session 7 Slides 8-11]

4.1 Cooling curves [Session 7 Slide 8]

Cooling curves are used to determine the temperatures of the phase transitions: the temperature of a cooling molten metal is recorded against time and plotted.

Cooling curves of pure iron and of a pure metal
Figure 7. Left: cooling curve of pure iron, with a thermal arrest at 1538, 1394 and 912 °C. Right: cooling curve of a pure metal: A to B cooling of the liquid, B solidification begins, C solidification ends, C to D cooling of the solid. Copied from Session 7 Slide 8.

4.2 Building the diagram from cooling curves [Session 7 Slide 9]

A binary isomorphous system has two components with complete solid solubility. Its diagram is built from the cooling curves of several compositions: each curve gives the temperature where solidification starts and the one where it ends. Joining the start points gives the liquidus; joining the end points gives the solidus. Above the liquidus everything is liquid (L), below the solidus everything is a single solid solution (SS), and between them liquid and solid coexist (L + SS).

0 % B 20 % B 50 % B 80 % B 100 % B cooling curves (T against time)
Figure 8. Cooling curves of alloys with 0, 20, 50, 80 and 100 % B: the pure components solidify at one temperature, the alloys between the start (liquidus) and the end (solidus) of solidification, the green points. Redrawn because on Session 7 Slide 9 the milk photographs cover the curves. Portal drawing, not in the slides (EXTRA)..
Isomorphous diagram
Figure 9. Binary isomorphous diagram: liquidus and solidus between the melting points of A and B, with the regions L, L + SS and SS. Copied from Session 7 Slide 9.

The slide compares the series of compositions with milk: whole, semi-skimmed and skimmed milk are mixtures of water and skim solids in different proportions, just as the alloys are mixtures of A and B.

4.3 Microstructure along the cooling [Session 7 Slide 10]

For an alloy of a given composition (the vertical line), the diagram tells what the microstructure is at each temperature:

Microstructure along the cooling of an isomorphous alloy
Figure 10. An alloy (system composition) cooled through the isomorphous diagram: all liquid L_system above the liquidus, crystallites of SS1 in a matrix of L1 at T1, and a polycrystalline solid SS_system below the solidus. Copied from Session 7 Slide 10.

The slide's analogy: milk alone is the liquid; milk with pieces of Manchego cheese is the two-phase mixture; the cheese alone is the solid.

4.4 Complete solid solubility [Session 7 Slide 11]

With complete solubility in the solid state:

Complete solid solubility
Figure 11. Isomorphous diagram with complete solid solubility from the melting point of A (1118 °C) to that of B (1553 °C), composition in mole fraction; the green dashed lines mark the alloys whose atom arrangements are shown below. Copied from Session 7 Slide 11.
Atomic arrangements of A-B solid solutions
Figure 12. Arrangement of A and B atoms in the same lattice for increasing B content: B atoms replace A atoms at any proportion. Copied from Session 7 Slide 11.

§ 5 Gibbs phase rule [Session 7 Slide 13]

The Gibbs phase rule counts how many variables can be changed independently while keeping the same phases in equilibrium:

$$F = C - P + N$$

With pressure and temperature both free, $N = 2$ and $F = C - P + 2$. For routine processing of materials the pressure can be considered fixed at 1 atm, so only temperature remains and

$$F = C - P + 1$$
Gibbs phase rule in a unary diagram
Figure 13. One component, F = C − P + 2: F = 2 in a single-phase region, 1 on a two-phase line and 0 at the triple point. Copied from Session 7 Slide 13.
Gibbs phase rule in a binary diagram
Figure 14. Two components at 1 atm, F = C − P + 1: F = 2 in L or in the solid, 1 in L + solid and on its boundaries, 0 at the melting point of a pure component. Copied from Session 7 Slide 13.
Worked example 2 — Counting degrees of freedom on the slide diagrams

One component (water), $F = 1 - P + 2$ [Session 7 Slide 13]:

  • inside a single-phase region (liquid): $F = 1 - 1 + 2 = 2$; temperature and pressure can both change without leaving the region;
  • on a two-phase line (for example solid-liquid): $F = 1 - 2 + 2 = 1$; if the temperature is chosen, the pressure is fixed by the line;
  • at the triple point: $F = 1 - 3 + 2 = 0$; three phases coexist only at one temperature and one pressure.

Two components at 1 atm, $F = 2 - P + 1$:

  • in L or in the solid solution: $F = 2 - 1 + 1 = 2$; temperature and composition can both change;
  • in L + solid (and on its boundaries): $F = 2 - 2 + 1 = 1$;
  • at the melting point of pure B, a single component with two phases: $F = 1 - 2 + 1 = 0$, which is why a pure metal melts at one fixed temperature.

Consequence for the tie line (§6). In the α + L region of the Cu-Ni diagram $F = 1$. Choosing the temperature uses that single degree of freedom, so the compositions of the two phases are no longer free: at about 1250 °C (a reading of the figure) they can only be $C_L$ = 32 wt% Ni and $C_\alpha$ = 43 wt% Ni [Session 7 Slide 16]. Changing the overall composition of the alloy changes only the amounts of the two phases, not their compositions.

§ 6 Tie line and lever rule [Session 7 Slides 15-21]

In a two-phase region two questions are answered with two tools [Session 7 Slide 15]:

Tie line and lever rule
Figure 15. Tie line through the alloy B (C_0) in the α + liquid region: it ends at C_L on the liquidus and at C_α on the solidus, and R and S are its two arms; Slide 16 prints C_L = 32, C_0 = 35 and C_α = 43 wt% Ni. Copied from Session 7 Slide 15.

For the alloy B, with overall composition $C_0$ and the arms $R = C_0 - C_L$ and $S = C_\alpha - C_0$:

$$W_L = \frac{S}{R + S} = \frac{C_\alpha - C_0}{C_\alpha - C_L} \qquad W_\alpha = \frac{R}{R + S} = \frac{C_0 - C_L}{C_\alpha - C_L} \qquad W_L + W_\alpha = 1$$

where $W_L$ is the mass fraction of liquid and $W_\alpha$ the mass fraction of α. They are mass fractions because the composition axis is in wt%; on an axis in atomic % the same construction gives atom (mole) fractions (extension, needed for the at.% diagrams of Problems 11-13 of the sheet).

Worked example 3 — Cu-35 wt% Ni at about 1250 °C [Session 7 Slides 16-21]

Data from the slide. $C_0 = 35$ wt% Ni at point B. The slide prints the three compositions but neither the temperature nor the name of the system: about 1250 °C is a reading of the figure (the tie line lies between the 1200 and 1300 °C grid lines), and "Cu-Ni" is assumed from the wt% Ni axis (extension). The tie line meets the liquidus at $C_L = 32$ wt% Ni and the solidus at $C_\alpha = 43$ wt% Ni.

Step 1, the arms of the lever. $R = C_0 - C_L = 35 - 32 = 3$ wt% Ni and $S = C_\alpha - C_0 = 43 - 35 = 8$ wt% Ni; the whole tie line is $R + S = C_\alpha - C_L = 43 - 32 = 11$ wt% Ni.

Step 2, the fractions. Each phase takes the arm on the side of the other phase:

$$W_L = \frac{S}{R+S} = \frac{43 - 35}{43 - 32} = \frac{8}{11} = 0.727 \qquad W_\alpha = \frac{R}{R+S} = \frac{35 - 32}{43 - 32} = \frac{3}{11} = 0.273$$

Step 3, checks. $W_L + W_\alpha = 8/11 + 3/11 = 1$. The nickel of the two phases adds up to the nickel of the alloy: $W_L C_L + W_\alpha C_\alpha = 0.727 \times 32 + 0.273 \times 43 = 23.27 + 11.73 = 35.0$ wt% Ni $= C_0$.

Answer. At about 1250 °C the alloy is 73 % liquid of 32 wt% Ni and 27 % solid α of 43 wt% Ni. The alloy point is closer to the liquidus, so there is more liquid.

Rounding on the slide

Slide 21 writes $W_L = 0.72$ and $W_\alpha = 0.28$. The exact values are $8/11 = 0.727$ and $3/11 = 0.273$, so they round to 0.73 and 0.27, as the official solutions of the problem sheet write them (Solution problems Phase diagrams I.pdf, p. 5). The slide truncates $W_L$ and then takes $W_\alpha = 1 - W_L$.

Worked example 4 — The same alloy during equilibrium cooling [Session 7 Slide 23]

Slide 23 prints the equilibrium compositions of the liquid and the solid at several temperatures for the same Cu-35 wt% Ni alloy. Applying the lever rule at each one:

Point$C_L$ (wt% Ni)$C_\alpha$ (wt% Ni)$W_L = \dfrac{C_\alpha - C_0}{C_\alpha - C_L}$$W_\alpha$
b′ (liquidus)3546$\dfrac{46 - 35}{46 - 35} = 1$0
c′2940$\dfrac{40 - 35}{40 - 29} = \dfrac{5}{11} = 0.455$0.545
d′ (solidus)2435$\dfrac{35 - 35}{35 - 24} = 0$1

Interpretation. At b′ the first solid appears, of 46 wt% Ni, in a liquid that still has the composition of the alloy. As the temperature falls both phases become poorer in Ni (the liquid follows the liquidus, the solid follows the solidus) and the amount of solid grows. At d′ the solid has reached the composition of the alloy, 35 wt% Ni, and the last liquid disappears: in equilibrium, solidification ends on the solidus.

§ 7 Non-equilibrium solidification [Session 7 Slides 23-24]

When the alloy goes down through the phase diagram too quickly (high cooling rates), solid-state diffusion has no time to keep the whole solid at the equilibrium composition. Only the surface of each growing crystal has the composition of the solidus; the inside keeps the composition it had when it formed. The result is a microstructure of heterogeneous composition, called microsegregation (or cored structure).

Non-equilibrium solidification of Cu-35 wt% Ni
Figure 16. Cooling of a Cu-35 wt% Ni alloy too fast for equilibrium: tie lines at b′, c′, d′ and e′, the cored crystals (46, 40, 35 and 31 wt% Ni from the centre out) and the dashed non-equilibrium solidus. Temperature (°C) against composition (wt% Ni). Copied from Session 7 Slide 23.

In the Cu-35 wt% Ni alloy the first solid is α of 46 wt% Ni (b′). At c′ the new layer is α of 40 wt% Ni, but the crystal still has its 46 % core, so its average composition is 42 wt% Ni instead of 40; at d′ the average is 38 instead of 35; at e′ it is 35. The average compositions follow a non-equilibrium solidus (dashed) that lies to the right of the equilibrium solidus, so liquid survives below the equilibrium solidus and solidification ends only at e′. The final grains are cored: 46 wt% Ni at the centre and 31 wt% Ni at the edge (f′).

The same behaviour in an alloy of Ni-30 wt% Cu (Slide 24): with fast cooling the solid follows the non-equilibrium solidus α′₂ … α′₇ and solidification ends at $T_7$ instead of $T_5$:

Equilibrium and non-equilibrium solidus of Ni-30 wt% Cu
Figure 17. Ni-30 wt% Cu alloy (labels in Spanish): with equilibrium cooling the solid follows α1 … α5 and solidification ends at T5; with fast cooling the average composition follows the non-equilibrium solidus α′2 … α′7 and it ends at T7. Copied from Session 7 Slide 24.
Cored crystals growing in the liquid at T2 and T4
Figure 18. Cored crystals of the Ni-30 % Cu alloy growing in the liquid at T₂ and T₄: each new layer (α′₁, α′₂, …) has a different composition. From Session 7 Slide 24.
Micrograph of a cored structure
Figure 19. Micrograph of a cored (microsegregated) structure: the rings in each grain are layers of different composition. From Session 7 Slide 24.

Removing the coring. Microsegregation can be eliminated with a homogenisation heat treatment at a temperature below the solidus (for example $T_{TT} < T_7$, below the lowest temperature at which liquid could exist). During the treatment, solid-state diffusion (Topic 3) evens out the composition inside the grains [Session 7 Slide 24].

Worked example 5 — How much liquid is left at d′ with fast cooling [Session 7 Slide 23]

Data from the slide. At d′ the liquid is $C_L$ = 24 wt% Ni, and the average composition of the cored solid is 38 wt% Ni (the dashed line). The alloy is $C_0$ = 35 wt% Ni.

Lever rule on the average composition. The tie line now ends on the non-equilibrium solidus, at 38 wt% Ni:

$$W_L = \frac{38 - 35}{38 - 24} = \frac{3}{14} = 0.214 \qquad W_\alpha = \frac{35 - 24}{38 - 24} = \frac{11}{14} = 0.786$$

Comparison. In equilibrium (Worked example 4) the alloy is completely solid at d′. With fast cooling about 21 % of the alloy is still liquid there; solidification ends only at e′, where the average composition of the solid reaches 35 wt% Ni and $W_L = (35 - 35)/(35 - 21) = 0$. The slide gives the average compositions; the lever rule is used here with them exactly as in §6.

§ 8 Binary eutectic systems [Session 7 Slides 26-32]

8.1 Partial solid solubility and the eutectic reaction [Session 7 Slides 26-27]

When the two components have only partial solid solubility, two solid solutions appear: α, rich in A, and β, rich in B. Their regions are bounded by three kinds of line:

Binary eutectic system
Figure 20. Binary eutectic diagram with liquidus, solidus and solvus, the regions L, α, β, α + L, L + β and α + β, the eutectic temperature and composition, and the eutectic microstructure of fine alternating layers of α and β. Copied from Session 7 Slide 26.

The two liquidus lines meet at the eutectic point, defined by the eutectic temperature and the eutectic composition. A liquid of eutectic composition does not pass through a two-phase L + solid region: at the eutectic temperature it transforms at once into two solids, in a fine microstructure of alternating layers of α and β.

Invariant reactions are produced at a fixed composition and a fixed temperature for a given system, and the result also remains fixed. In a system of two partially soluble components, a solidification reaction occurs at a fixed composition and temperature, with a cooling curve similar to that of a pure solid [Session 7 Slide 27]. This is the eutectic reaction:

$$L \;\rightarrow\; \alpha + \beta \quad \text{(on cooling, at the eutectic temperature)}$$
Cooling curve of the eutectic alloy and the eutectic reaction
Figure 21. Cooling curve at the eutectic temperature (183 °C plateau; axes in Spanish, Temperatura and Tiempo) and the shape of the eutectic reaction L → α + β on the diagram. Copied from Session 7 Slide 27.

With the phase rule of §5 at 1 atm: at the eutectic point three phases (L, α, β) coexist in a two-component system, so $F = 2 - 3 + 1 = 0$. Temperature and the compositions of the three phases are all fixed, which is why the reaction is invariant and the cooling curve shows a plateau.

8.2 The Pb-Sn system and the eutectic microstructure [Session 7 Slides 28-29]

The Pb-Sn diagram is the example of the slides. Its eutectic point is at 61.9 wt% Sn and 183 °C. At 183 °C, α can dissolve at most 18.3 wt% Sn and β contains 97.8 wt% Sn [Session 7 Slides 27, 32]. The melting points of the pure metals are 327 °C (Pb) and 232 °C (Sn) (Problems T4_PhaseDiagrams I.pdf, p. 1).

The Pb-Sn eutectic system
Figure 22. Pb-Sn phase diagram (axes in Spanish: Temperatura, Peso porcentual de estaño) with the eutectic at about 61.9 wt% Sn and 183 °C; the thick arrows point to the sketches of the eutectic reaction shown below. Copied from Session 7 Slide 28.

A liquid of 61.9 wt% Sn, cooled to 183 °C, forms colonies of α and β layers that grow together into the liquid until the whole structure is eutectic (the eutectic product). The layers alternate with a spacing λ:

Eutectic forming from the liquid in Pb-Sn
Figure 23. Pb-Sn eutectic: layers of α and β grow together from the liquid of 61.9 % Sn (top) until the whole structure is eutectic colonies (bottom). From Session 7 Slide 28.
Lamellae of the eutectic product
Figure 24. The eutectic product: alternating lamellae of α and β; λ is the spacing of the layers. From Session 7 Slide 28.
Micrograph of the Pb-Sn eutectic
Figure 25. Micrograph of the Pb-Sn eutectic (scale bar 40 µm): dark and light layers are the two phases. From Session 7 Slide 28.

The shape of the eutectic changes from one system to another, as the four micrographs of Slide 29 show (Sn-50In, Al-13Si, Al-33Cu and Mg-37Sn): in them one phase appears as rods, plates, globules or needles inside the other (a description of those micrographs).

Eutectic microstructures of four alloys
Figure 26. Eutectic microstructures: (a) Sn-50 % In, (b) Al-13 % Si, (c) Al-33 % Cu, (d) Mg-37 % Sn. From Session 7 Slide 29.
Pb-Sn values in the problem sheet

The diagram printed in the problem sheet (Problems T4_PhaseDiagrams I.pdf, p. 1) and the official solutions use 19.2 wt% Sn for α and 97.5 wt% Sn for β at 183 °C, instead of the 18.3 and 97.8 of Slide 32: they come from a different drawing of the same system. The worked examples of this page use the slide values; the solved problems use the values of the sheet.

Worked example 6 — Phases in the Pb-Sn eutectic product [Session 7 Slides 28, 32]

Question. A Pb-61.9 wt% Sn alloy (eutectic composition) is cooled just below 183 °C. What are the amounts of α and β in the eutectic?

Tie line. Just below 183 °C the tie line crosses the α + β region from $C_\alpha$ = 18.3 to $C_\beta$ = 97.8 wt% Sn; its length is $97.8 - 18.3 = 79.5$ wt% Sn.

Lever rule.

$$W_\alpha = \frac{C_\beta - C_0}{C_\beta - C_\alpha} = \frac{97.8 - 61.9}{97.8 - 18.3} = \frac{35.9}{79.5} = 0.452 \qquad W_\beta = \frac{C_0 - C_\alpha}{C_\beta - C_\alpha} = \frac{61.9 - 18.3}{79.5} = \frac{43.6}{79.5} = 0.548$$

Check. $0.452 + 0.548 = 1$ and $0.452 \times 18.3 + 0.548 \times 97.8 = 8.27 + 53.59 = 61.9$ wt% Sn $= C_0$.

Answer. The alloy is 100 % eutectic microconstituent, and inside it 45.2 % of the mass is α and 54.8 % is β. Every eutectic of this system, whatever the alloy it comes from, has these proportions (used in Worked example 7).

8.3 Hypoeutectic and hypereutectic alloys [Session 7 Slides 30-31]

An alloy between the α limit and the eutectic composition is hypoeutectic; one between the eutectic composition and the β limit is hypereutectic.

Hypoeutectic alloy (the slide uses Pb-Sn with about 30 wt% Sn, a reading of the figure):

Hypoeutectic Pb-Sn alloy on the diagram
Figure 27. Pb-Sn diagram with the dashed line of the hypoeutectic alloy (about 30 wt% Sn); the arrows point to the microstructure sketches shown below. Copied from Session 7 Slide 30.
Cooling curve of a hypoeutectic alloy
Figure 28. Cooling curve of the hypoeutectic alloy: liquidus at 260 °C, α + L, the eutectic plateau at 183 °C (L → α + β) and α + eutectic below it. Copied from Session 7 Slide 30.
  1. Above the liquidus the alloy is liquid. The cooling curve shows the liquidus at 260 °C, where crystals of α start to form.
  2. Between 260 and 183 °C, α and liquid coexist; α grows, and the liquid becomes richer in Sn along the liquidus.
  3. Just above 183 °C the solid is α of 18.3 wt% Sn and the liquid has reached the eutectic composition, 61.9 wt% Sn.
  4. At 183 °C that liquid transforms at constant temperature into the eutectic ($L \rightarrow \alpha + \beta$): a plateau in the cooling curve.
  5. Below 183 °C the structure is primary (proeutectic) α surrounded by eutectic.
Microstructure of a hypoeutectic Pb-Sn alloy during cooling
Figure 29. Hypoeutectic Pb-Sn alloy, from top to bottom: α crystals in the liquid; α of 19 % Sn in liquid of 61.9 % Sn just above the eutectic temperature; eutectic forming around the α; primary α in a eutectic matrix. From Session 7 Slide 30.
Micrograph of a hypoeutectic Pb-Sn alloy
Figure 30. Micrograph of a hypoeutectic Pb-Sn alloy: dark rounded primary α in the lamellar eutectic. From Session 7 Slide 30.

In a casting, the primary α grows from the mould wall, and the liquid trapped between the crystals is the last to solidify, with the eutectic composition:

Hypoeutectic solidification in a mould
Figure 31. Hypoeutectic solidification in a mould: primary α grows from the mould wall and the last liquid, between the crystals, reaches the eutectic composition. From Session 7 Slide 30.

Hypereutectic alloy: the same sequence with the roles of the solids exchanged. Primary β forms between the liquidus and the eutectic temperature, the remaining liquid gives the eutectic at the eutectic temperature, and the final structure is primary β plus eutectic.

Hypereutectic alloy on the diagram
Figure 32. Eutectic diagram with the dashed line of a hypereutectic alloy and its points in L, L + β and α + β; the arrows point to the microstructure sketches shown below. Copied from Session 7 Slide 31.
Cooling curve of a hypereutectic alloy
Figure 33. Cooling curve of the hypereutectic alloy: primary β forms below the liquidus, then the eutectic plateau (L → α + β) and β + eutectic below it; the slide repeats the labels 260 and 183 °C of the hypoeutectic curve. Copied from Session 7 Slide 31.
Microstructure of a hypereutectic alloy during cooling
Figure 34. Hypereutectic alloy, from top to bottom: β crystals in the liquid; primary β just above the eutectic temperature; primary β in a eutectic matrix. From Session 7 Slide 31.
Micrograph of a hypereutectic alloy
Figure 35. Micrograph of a hypereutectic alloy: light rounded primary β in the eutectic. From Session 7 Slide 31.

(The cooling curve of Slide 31 repeats the temperature labels of the hypoeutectic curve, 260 and 183 °C; for a hypereutectic Pb-Sn alloy the liquidus is below 232 °C, so read them only as the liquidus temperature $T_L$ and the eutectic temperature $T_E$ of the alloy.)

8.4 Lever rule in binary eutectic diagrams [Session 7 Slide 32]

Just below the eutectic temperature, the tie line of a hypoeutectic alloy $C'_4$ is cut by the alloy and by the eutectic composition into three segments, $P$, $Q$ and $R$:

Lever rule in the Pb-Sn eutectic diagram
Figure 36. Pb-Sn diagram with the segments P, Q and R of the tie line just below 183 °C, from 18.3 wt% Sn (α) through the alloy C′4 and the eutectic 61.9 wt% Sn to 97.8 wt% Sn (β). Copied from Session 7 Slide 32.
$$W_{\alpha'} = \frac{Q}{P + Q} \qquad W_e = W_L = \frac{P}{P + Q} \qquad W_\alpha = \frac{Q + R}{P + Q + R} \qquad W_\beta = \frac{P}{P + Q + R}$$

The first two use the short tie line between α and the eutectic liquid (microconstituents); the last two use the whole tie line between α and β (phases).

Worked example 7 — Microconstituents and phases of Pb-30 wt% Sn [Session 7 Slides 30, 32]

Data. Alloy $C_0$ = 30 wt% Sn (the hypoeutectic alloy of Slide 30), just below 183 °C, with the values of Slide 32: $C_\alpha$ = 18.3, $C_e$ = 61.9, $C_\beta$ = 97.8 wt% Sn.

Step 1, the segments. $P = C_0 - C_\alpha = 30 - 18.3 = 11.7$; $Q = C_e - C_0 = 61.9 - 30 = 31.9$; $R = C_\beta - C_e = 97.8 - 61.9 = 35.9$; so $P + Q = 43.6$ and $P + Q + R = 79.5$ (all in wt% Sn).

Step 2, microconstituents (short tie line, from α to the eutectic liquid):

$$W_{\alpha'} = \frac{Q}{P+Q} = \frac{31.9}{43.6} = 0.732 \qquad W_e = \frac{P}{P+Q} = \frac{11.7}{43.6} = 0.268$$

Step 3, phases (whole tie line, from α to β):

$$W_\alpha = \frac{Q+R}{P+Q+R} = \frac{67.8}{79.5} = 0.853 \qquad W_\beta = \frac{P}{P+Q+R} = \frac{11.7}{79.5} = 0.147$$

Step 4, the α inside the eutectic. It is the total α minus the primary α: $W_{\alpha,e} = W_\alpha - W_{\alpha'} = 0.853 - 0.732 = 0.121$.

Check, phases against microconstituents. By Worked example 6 every eutectic is 45.2 % α and 54.8 % β. Then $W_e \times 0.452 = 0.268 \times 0.452 = 0.121 = W_{\alpha,e}$ and $W_e \times 0.548 = 0.268 \times 0.548 = 0.147 = W_\beta$: both descriptions of the alloy agree.

Answer. Just below 183 °C the alloy is 73.2 % primary α and 26.8 % eutectic. Counting phases, it is 85.3 % α (73.2 % primary plus 12.1 % in the eutectic) and 14.7 % β. Just above 183 °C the same lever gives 73.2 % α of 18.3 wt% Sn and 26.8 % liquid of 61.9 wt% Sn: that liquid is what becomes the eutectic.

Part II — Phase diagrams II (Session 8)

§ 9 Solid-state precipitation [Session 8 Slides 2-4]

9.1 Below the solid solubility limit [Session 8 Slide 2]

An alloy whose composition stays inside the α region all the way down to room temperature never crosses the solvus: once solid, it is single-phase α. In the Pb-Sn example, a Pb-1 wt% Sn alloy ($C_1$) is:

Pb-1 wt% Sn below the solvus
Figure 37. Pb-Sn diagram with the alloy C1 (1 wt% Sn) and its microstructures at a (liquid), b (α + L) and c (only α). Copied from Session 8 Slide 2.
Pb-16 wt% Sn crossing the solvus
Figure 38. Pb-Sn diagram with the alloy C2 (16 wt% Sn) and its microstructures at d (liquid), e (α + L), f (only α) and g (α + β precipitates after crossing the solvus line). Copied from Session 8 Slide 4.

9.2 Above the solid solubility limit: precipitation [Session 8 Slides 3-4]

Precipitation in the solid state: when an alloy crosses the solvus line on cooling, the solid solubility of α is exceeded, and small particles of the β phase form; they grow as the temperature decreases [Session 8 Slide 3].

Solid-state precipitation in an alloy of 20 % B
Figure 39. Cooling of an alloy of 20 % B: all liquid, α1 in a matrix of L1, all α, and β2 particles in a matrix of α2 after crossing the solvus (the slide prints '00%' for 100 %). Copied from Session 8 Slide 3.

For the alloy of 20 % B of the slide: all liquid; α₁ crystals in a matrix of liquid L₁; 100 % α with the composition of the alloy; and, below the solvus, small β₂ particles in a matrix of α₂ (mostly at the grain boundaries), which become more and grow at lower temperatures (α₃ + β₃).

Micrograph of precipitates at grain boundaries
Figure 40. Micrograph of solid-state precipitates at the grain boundaries (scale bar 20 µm). From Session 8 Slide 3.

The Pb-Sn example of Slide 4 uses a Pb-16 wt% Sn alloy ($C_2$, also in the figure of §9.1):

Micrographs of precipitates inside the grains
Figure 41. Precipitates inside the grains; on the right, a detail of the circled area. From Session 8 Slide 4.
Worked example 8 — How much β precipitates in Pb-16 wt% Sn [Session 8 Slide 4]

Readings of the figure. On Slide 4 the vertical line of $C_2$ = 16 wt% Sn meets the solvus at about 172 °C; at point g (121 °C) the solvus is at about 6 wt% Sn. The β boundary at that temperature is close to pure Sn; Slide 32 of Session 7 places it at about 99 wt% Sn.

Above about 172 °C (point f, 192 °C) the alloy is single-phase α of 16 wt% Sn: $W_\alpha = 1$.

At 121 °C (point g), lever rule on the tie line from 6 to 99 wt% Sn:

$$W_\beta = \frac{C_0 - C_\alpha}{C_\beta - C_\alpha} = \frac{16 - 6}{99 - 6} = \frac{10}{93} = 0.108 \qquad W_\alpha = \frac{99 - 16}{99 - 6} = \frac{83}{93} = 0.892$$

Interpretation. About 11 % of the alloy has turned into β particles between 172 and 121 °C. As the temperature falls further the solvus moves to lower Sn contents, so the α holds less Sn and more β precipitates: the particles grow, as the slide says. These numbers depend on readings of the figure and are approximate.

§ 10 Invariant reactions [Session 8 Slides 6-12]

10.1 The five reactions [Session 8 Slide 6]

An invariant reaction happens at a fixed temperature, with fixed compositions of the three phases involved ($F = 2 - 3 + 1 = 0$ at constant pressure, §5). The slides list five types; the eutectoid and the peritectoid happen entirely in the solid state:

The five invariant reactions of binary diagrams
Figure 42. Eutectic, peritectic, monotectic, eutectoid and peritectoid reactions with their equations on cooling and their shape on the diagram; the last two are solid-state reactions. Copied from Session 8 Slide 6.
ReactionOn coolingShape on the diagram
Eutectic$L \rightarrow \alpha + \beta$a liquid region ends in a V on the horizontal line
Peritectic$\alpha + L \rightarrow \beta$a solid region ends in an inverted V below the line
Monotectic$L_1 \rightarrow L_2 + \alpha$a liquid miscibility gap above the line
Eutectoid$\gamma \rightarrow \alpha + \beta$like the eutectic, with a solid γ instead of L
Peritectoid$\alpha + \beta \rightarrow \gamma$like the peritectic, with two solids

10.2 Eutectoid reaction [Session 8 Slide 7]

Eutectoid reaction: an invariant reaction where a solid phase transforms into two solid phases: $\gamma \rightarrow \alpha + \beta$.

Example, Cu-Zn at 560 °C (74 % Zn; here and in the next examples the slides print the compositions as % of the second element, with no basis):

$$\delta\,(74\%\,\text{Zn}) \;\underset{\text{heating}}{\overset{\text{cooling}}{\rightleftharpoons}}\; \gamma\,(70\%\,\text{Zn}) + \varepsilon\,(78\%\,\text{Zn})$$
The eutectoid point of the Cu-Zn system
Figure 43. Detail of the Cu-Zn diagram around the eutectoid point E (560 °C, about 74 % Zn), where δ gives γ + ε, and the peritectic point P (598 °C). Copied from Session 8 Slide 7.
Micrograph of the Cu-Zn eutectoid structure
Figure 44. Micrograph of the eutectoid product of the Cu-Zn alloy, a fine mixture of γ and ε. From Session 8 Slide 7.
Worked example 9 — The Cu-Zn eutectoid product [Session 8 Slide 7]

Question. A Cu-74 wt% Zn alloy (all δ) is cooled just below 560 °C. How much γ and how much ε does it contain?

Lever rule on the tie line from γ (70 % Zn) to ε (78 % Zn), length $78 - 70 = 8$:

$$W_\gamma = \frac{C_\varepsilon - C_0}{C_\varepsilon - C_\gamma} = \frac{78 - 74}{78 - 70} = \frac{4}{8} = 0.50 \qquad W_\varepsilon = \frac{C_0 - C_\gamma}{C_\varepsilon - C_\gamma} = \frac{74 - 70}{8} = 0.50$$

Check: $0.50 \times 70 + 0.50 \times 78 = 74$ % Zn. Answer: the eutectoid product is half γ and half ε, a fine mixture of the two solids, as in the micrograph. On heating the reaction runs backwards and the mixture turns into single-phase δ.

10.3 Peritectic reaction [Session 8 Slides 8-9]

Peritectic reaction: an invariant reaction where a solid and a liquid phase transform into a different solid phase, $\alpha + L \rightarrow \beta$. The peritectic point is the invariant point where this happens [Session 8 Slide 8].

A peritectic point
Figure 45. Generic peritectic diagram: the reaction α + L → β at the peritectic point P, temperature T_P, between the points a and b. Copied from Session 8 Slide 8.

Example, Fe-Ni at 1517 °C and 4.3 % Ni:

$$\delta\,(4.0\%\,\text{Ni}) + L\,(5.4\%\,\text{Ni}) \;\xrightarrow[\text{cooling}]{1517^\circ\text{C}}\; \gamma\,(4.3\%\,\text{Ni})$$
The peritectic point of the Fe-Ni system
Figure 46. Fe-Ni diagram near the peritectic at 1517 °C: δ (4.0 % Ni) + L (5.4 % Ni) → γ (4.3 % Ni), with the points a, b and c of the 4.3 % Ni alloy. Copied from Session 8 Slide 8.
Worked example 10 — Fe-4.3 wt% Ni around 1517 °C [Session 8 Slide 8]

Just above 1517 °C the alloy is δ (4.0 % Ni) + L (5.4 % Ni); tie line length $5.4 - 4.0 = 1.4$:

$$W_\delta = \frac{5.4 - 4.3}{5.4 - 4.0} = \frac{1.1}{1.4} = 0.786 \qquad W_L = \frac{4.3 - 4.0}{1.4} = \frac{0.3}{1.4} = 0.214$$

Just below 1517 °C both react and give γ of 4.3 % Ni, the composition of the alloy, so the alloy is 100 % γ.

Check: $0.786 \times 4.0 + 0.214 \times 5.4 = 3.14 + 1.16 = 4.30$ % Ni. The liquid and the δ are used up together because the alloy has exactly the peritectic composition.

Second example, Pt-Ag at 1186 °C (42.4 % Ag) [Session 8 Slide 9]:

The peritectic reaction in the Pt-Ag system
Figure 47. Pt-Ag diagram with alloy 1 (42.4 % Ag) and alloy 2 (about 60 % Ag), the tie lines at 1400 °C and 1150 °C and the peritectic line at 1186 °C; the arrows lead to the microstructure sketches of the slide. Copied from Session 8 Slide 9.
Microstructure during the peritectic reaction
Figure 48. Peritectic reaction with decreasing temperature: α crystals in liquid; β forms around them; all β. From Session 8 Slide 9.
Worked example 11 — The Pt-Ag peritectic, alloys 1 and 2 [Session 8 Slide 9]

Alloy 1, 42.4 % Ag, at 1400 °C. Liquid (55 % Ag) + α (7 % Ag); tie line length $55 - 7 = 48$:

$$W_L = \frac{42.4 - 7}{55 - 7} = \frac{35.4}{48} = 0.7375 \qquad W_\alpha = \frac{55 - 42.4}{48} = \frac{12.6}{48} = 0.2625$$

Alloy 1 at 1186 °C + ΔT. Liquid (66.3 % Ag) + α (10.5 % Ag); length $66.3 - 10.5 = 55.8$:

$$W_L = \frac{42.4 - 10.5}{66.3 - 10.5} = \frac{31.9}{55.8} = 0.572 \qquad W_\alpha = \frac{66.3 - 42.4}{55.8} = \frac{23.9}{55.8} = 0.428$$

Alloy 1 at 1186 °C − ΔT. Only β, of 42.4 % Ag: 100 %. The liquid and the α have reacted completely ($\alpha + L \rightarrow \beta$).

Alloy 2 (about 60 % Ag, a reading of the figure) at 1150 °C: L + β, with the tie line of the slide from β (48 % Ag) to L (77 % Ag), length 29:

$$W_\beta = \frac{77 - 60}{77 - 48} = \frac{17}{29} = 0.586 \qquad W_L = \frac{60 - 48}{29} = \frac{12}{29} = 0.414$$

Alloy 2 has more Ag than the peritectic composition, so after the peritectic reaction some liquid is left (L + β); it solidifies completely on further cooling.

Formula on Slide 9

For 1186 °C + ΔT the slide writes "Alpha: (66.3 − 10.5)/(66.3 − 10.5) = 43 %". The numerator must be $66.3 - 42.4 = 23.9$ (the arm on the side of the liquid); $(66.3 - 10.5)/(66.3 - 10.5)$ would be 1. The value 43 % is right.

Rapid (non-equilibrium) solidification in peritectic systems [Session 8 Slide 10]:

Rapid solidification in a peritectic system
Figure 49. Rapid (non-equilibrium) solidification of alloy X: the solid follows non-equilibrium compositions (α′, β′) and the peritectic reaction is incomplete. From Session 8 Slide 10.
β surrounding primary α during the peritectic reaction
Figure 50. Encasement: the β formed by the peritectic reaction surrounds the primary α, so B atoms from the liquid and A atoms from α must diffuse through it. From Session 8 Slide 10.

10.4 Peritectoid reaction [Session 8 Slide 11]

Peritectoid reaction: an invariant reaction where two solid phases transform into a new solid phase, $\beta + \alpha \rightarrow \gamma$. The peritectoid point is the invariant point where it happens.

A peritectoid point
Figure 51. Generic peritectoid diagram: the solids α and β react to give γ at the circled peritectoid point. Copied from Session 8 Slide 11.
The Co-W phase diagram with a peritectoid point
Figure 52. Co-W diagram: the arrow marks a peritectoid point, where two solid phases give the new solid γ. From Session 8 Slide 11.

10.5 Monotectic reaction [Session 8 Slide 12]

Monotectic reaction: an invariant reaction where a liquid phase transforms into a solid phase plus another liquid (the liquid has a miscibility gap): $L_1 \rightarrow L_2 + \alpha$. The monotectic point is the invariant point where this happens.

Example, Cu-Pb at 955 °C (36 % Pb):

$$L\,(36\%\,\text{Pb}) \;\underset{\text{heating}}{\overset{\text{cooling}}{\rightleftharpoons}}\; L_2\,(87\%\,\text{Pb}) + \alpha\,(0\%\,\text{Pb})$$
The monotectic reaction in the Cu-Pb system
Figure 53. Cu-Pb diagram with the monotectic at 955 °C (36 % Pb, the blue dot), the miscibility gap of the liquid up to 991 °C and the line at 326 °C. Copied from Session 8 Slide 12.
Worked example 12 — Cu-36 wt% Pb just below 955 °C [Session 8 Slide 12]

Tie line from α (0 % Pb) to $L_2$ (87 % Pb), length 87:

$$W_\alpha = \frac{87 - 36}{87 - 0} = \frac{51}{87} = 0.586 \qquad W_{L_2} = \frac{36 - 0}{87} = \frac{36}{87} = 0.414$$

Interpretation. Just below 955 °C the alloy is 59 % solid copper and 41 % of a second liquid, rich in lead (87 %). That liquid stays liquid down to 326 °C, where $L_2$ undergoes a eutectic reaction, $L_2 \rightarrow \alpha + \beta$ (a reading of the diagram, which shows the 326 °C line with α + β below it; the slide text does not name it); the slide's diagram shows the region α + L₂ between the two lines.

§ 11 Intermetallic compounds [Session 8 Slides 14-15]

An intermetallic compound is made up of two or more elements (components) and produces a new phase with its own composition, crystal structure and properties [Session 8 Slides 14-15].

Terminal and intermediate phases
Figure 54. A diagram with terminal phases (α, ζ) at the ends and intermediate phases (β, γ, δ, ε) inside, around the compounds A₂B, AB, AB₂ and AB₄. From Session 8 Slide 14.

Two kinds of compound [Session 8 Slide 15]:

The Ti-B diagram of the slides
Figure 55. Ti-B: Ti₃B₄ is a stoichiometric compound (a vertical line); TiB and TiB₂ have a range of compositions. From Session 8 Slide 15.
Composition axis of Slide 15

The label under the Ti-B diagram of Slide 15 reads "% wt Boron", but the compounds sit at about 50 % (TiB) and 67 % ($\text{TiB}_2$), which are their atomic percentages (one B per Ti, two B per Ti). The same diagram in the problem sheet (Problems T4_PhaseDiagrams I.pdf, p. 7) has the atomic scale on top and the weight scale below, where TiB is at about 18 wt% and $\text{TiB}_2$ at about 31 wt% B.

§ 12 Congruent and incongruent melting [Session 8 Slide 17]

Congruent and incongruent melting in the Mg-Ni system
Figure 56. Mg-Ni diagram: MgNi2 melts congruently (at a maximum of the liquidus) and Mg2Ni incongruently (it ends at a horizontal peritectic line). Copied from Session 8 Slide 17.

On the diagram, a congruently melting compound sits at a maximum of the liquidus (it melts at a single temperature, like a pure metal), while an incongruently melting one ends at a horizontal peritectic line.

Worked example 13 — Classifying the Ti-B compounds [Session 8 Slides 15, 17]

Reading the Ti-B diagram of Slide 15:

  • $\text{TiB}_2$ reaches the top of the liquidus dome, at 3225 °C: the liquid formed there has the same composition as the solid, so $\text{TiB}_2$ melts congruently.
  • $\text{Ti}_3\text{B}_4$ and TiB end at horizontal lines near 2200 °C, below the liquidus: on heating, each gives liquid plus a different solid (for $\text{Ti}_3\text{B}_4$, liquid + $\text{TiB}_2$). Both melt incongruently; on cooling they form by peritectic reactions.

This is the classification used in Problem 15 of the sheet.

Part III — Phase diagrams III: the Fe-C system (Session 9)

§ 13 The Fe-C system [Session 9 Slides 2-11]

13.1 Why it matters [Session 9 Slide 2]

Micrographs of two steels
Figure 57. Different microstructures in the Fe-C system. From Session 9 Slide 2.

13.2 Allotropic phases of pure iron [Session 9 Slide 3]

Allotropy is the existence of a chemical element in two or more forms, which may differ in the arrangement of the atoms in the crystalline solid (Topic 2). Iron undergoes two changes of crystal structure before it melts:

Allotropic phases of pure iron
Figure 58. Allotropic phases of pure iron from room temperature to the liquid: Fe-α (BCC) up to 910 °C, Fe-γ (FCC) up to 1390 °C and Fe-δ (BCC) up to 1535 °C. Copied from Session 9 Slide 3.
FCC and BCC cells of iron
Figure 59. Unit cells of Fe-γ (FCC, top) and Fe-α (BCC, bottom). From Session 9 Slide 3.

The temperatures on the scale of Slide 3 (910, 1390 and 1535 °C) differ by a few degrees from those printed on the Fe-C diagram of the same session (912, 1394 and 1538 °C, Slide 4); the diagram values are used in the rest of this page.

13.3 The Fe-Fe₃C diagram [Session 9 Slide 4]

The diagram used in practice is metastable: its right-hand end is 6.67 wt% C, the stoichiometric composition of Fe₃C, iron carbide or cementite. So the diagram is in fact Fe-Fe₃C. It has three invariant points (a peritectic, a eutectic and a eutectoid), and its composition axis is split into four ranges:

The metastable Fe-Fe3C phase diagram
Figure 60. Fe-Fe3C diagram up to 6.67 wt% C with the peritectic, eutectic (4.30 % C, 1147 °C) and eutectoid (0.76 % C, 727 °C) points marked, the limit 2.14 % C, and the ranges of hypoeutectoid and hypereutectoid steels and of hypoeutectic and hypereutectic cast irons. Copied from Session 9 Slide 4.
RangeName
up to 0.76 % Chypoeutectoid steels
0.76 to 2.14 % Chypereutectoid steels
2.14 to 4.30 % Chypoeutectic cast irons
4.30 to 6.67 % Chypereutectic cast irons

Steels have up to 2.14 % C; cast irons have more [Session 9 Slide 4].

13.4 Phases [Session 9 Slides 5-9]

Ferrite: BCC cell and micrograph
Figure 61. α-ferrite: BCC cell and micrograph of its grains. From Session 9 Slide 5.
Austenite: FCC cell with a carbon atom and micrograph
Figure 62. Austenite: FCC cell with a C atom in an interstitial site, and micrograph. From Session 9 Slide 6.
Unit cell of cementite
Figure 63. Unit cell of cementite, Fe₃C. From Session 9 Slide 8.

Austenite dissolves much more carbon than ferrite (2.14 against 0.022 wt%), because the interstitial sites of FCC iron are larger than those of BCC iron (extension: the Session 9 slides state the solubilities but not this reason).

Two-phase regions [Slide 9]: α-ferrite + Fe₃C below 727 °C; γ-austenite + Fe₃C between 727 and 1147 °C.

13.5 Invariant reactions [Session 9 Slide 10]

ReactionEquation (wt% C)Product
Eutectoid, 727 °C$\gamma\,(0.76) \rightleftharpoons \alpha\,(0.022) + \text{Fe}_3\text{C}\,(6.67)$pearlite
Eutectic, 1147 °C$L\,(4.3) \rightleftharpoons \gamma\,(2.14) + \text{Fe}_3\text{C}\,(6.67)$ledeburite
Peritectic, 1493 °C$\delta\,(0.09) + L\,(0.53) \rightleftharpoons \gamma\,(0.16)$austenite
Worked example 14 — The make-up of ledeburite [Session 9 Slide 10]

Question. How much austenite and how much cementite does the eutectic product of Fe-C (ledeburite) contain just below 1147 °C?

Tie line from γ (2.14 % C) to Fe₃C (6.67 % C), length $6.67 - 2.14 = 4.53$; the liquid had $C_0 = 4.30$ % C:

$$W_{\text{Fe}_3\text{C}} = \frac{C_0 - C_\gamma}{C_{\text{Fe}_3\text{C}} - C_\gamma} = \frac{4.30 - 2.14}{6.67 - 2.14} = \frac{2.16}{4.53} = 0.477 \qquad W_\gamma = \frac{6.67 - 4.30}{4.53} = \frac{2.37}{4.53} = 0.523$$

Check: $0.523 \times 2.14 + 0.477 \times 6.67 = 1.12 + 3.18 = 4.30$ % C. Answer: ledeburite is about 52 % austenite and 48 % cementite. Below 727 °C its austenite becomes pearlite ("transformed ledeburite", Slide 11).

13.6 Microconstituents [Session 9 Slide 11]

The microconstituents of the system are pearlite, proeutectoid ferrite and proeutectoid cementite in steels, and ledeburite (transformed below 727 °C) with cementite and pearlite in cast irons. The lines of the diagram have names used in heat treatment: $A_1$ is the eutectoid line (727 °C), $A_3$ the boundary between γ and α + γ, and $A_{cm}$ the boundary between γ and γ + Fe₃C.

Microconstituents of the Fe-C system
Figure 64. Microconstituents of the Fe-C system: pearlite, ferrite and cementite in steels; ledeburite in cast irons. The figure uses older values (0.83 % C, 723 and 1130 °C). From Session 9 Slide 11.

§ 14 Equilibrium transformations of steels [Session 9 Slides 12-20]

14.1 Eutectoid steels, $C_0$ = 0.76 % C [Session 9 Slides 12-13]

Pearlitic transformation: austenite of 0.76 % C gives a single microconstituent, pearlite, formed by layers (lamellae) of two phases, α + Fe₃C [Slide 12].

Cooling of a eutectoid steel (0.76 % C)
Figure 65. Eutectoid steel: at a (above 727 °C) only austenite; at b (just below 727 °C) the austenite has become pearlite, layers of α and Fe3C. Copied from Session 9 Slide 12.
Micrograph of pearlite
Figure 66. Pearlite: alternating layers of ferrite (light) and cementite (dark). From Session 9 Slide 12.

Ferrite nucleates on the grain boundaries of the austenite and displaces the carbon to the neighbouring zones by diffusion; there cementite forms. Decreasing the spacing of the pearlite lamellae increases its hardness [Slide 12].

Growth of pearlite
Figure 67. Growth of pearlite from an austenite grain boundary: ferrite rejects carbon, which diffuses to the neighbouring zones where cementite forms. From Session 9 Slide 12.
Worked example 15 — Phases of a eutectoid steel at point b [Session 9 Slide 13]

Point b (just below 727 °C): one microconstituent, pearlite; two phases, ferrite ($C_\alpha$ = 0.022 % C) and cementite ($C_{\text{Fe}_3\text{C}}$ = 6.67 % C). Tie line length $6.67 - 0.022 = 6.648$:

$$W_\alpha = \frac{C_{\text{Fe}_3\text{C}} - C_0}{C_{\text{Fe}_3\text{C}} - C_\alpha} = \frac{6.67 - 0.76}{6.67 - 0.022} = \frac{5.91}{6.648} = 0.889 \qquad W_{\text{Fe}_3\text{C}} = 1 - 0.889 = 0.111$$

Check: $0.889 \times 0.022 + 0.111 \times 6.67 = 0.020 + 0.740 = 0.76$ % C. Answer: pearlite is 89 % ferrite and 11 % cementite, as on the slide. Every pearlite, in any steel, has this make-up.

14.2 Hypoeutectoid steels, $C_0$ < 0.76 % C [Session 9 Slides 14-18]

Two microconstituents: pearlite and proeutectoid (primary) ferrite, $\alpha_P$ [Slide 14].

Cooling of a hypoeutectoid steel (0.3 % C)
Figure 68. Hypoeutectoid steel C0: c only γ; d and e, proeutectoid α growing at the γ grain boundaries between the A3 line M-O and 727 °C; f, proeutectoid α and pearlite. Copied from Session 9 Slide 14.
Micrograph of a hypoeutectoid steel
Figure 69. Hypoeutectoid steel: light proeutectoid (primary) ferrite and dark pearlite. From Session 9 Slide 14.

On cooling a steel of 0.3 % C: at c it is only γ; between the $A_3$ line (M-O) and 727 °C ferrite nucleates at the austenite grain boundaries and grows (d, e) while the austenite becomes richer in carbon along $A_3$; at 727 °C the remaining austenite, now of 0.76 % C, becomes pearlite (f).

Worked example 16 — A 0.3 % C steel at points c, d, e and f [Session 9 Slides 15-18]

Point c: one phase, austenite, $C_\gamma = C_0 = 0.3$ % C, $W_\gamma = 100$ %.

Point d: ferrite ($C_\alpha$ = 0.02 % C) and austenite ($C_\gamma$ = 0.4 % C), length 0.38:

$$W_\alpha = \frac{C_\gamma - C_0}{C_\gamma - C_\alpha} = \frac{0.4 - 0.3}{0.4 - 0.02} = \frac{0.1}{0.38} = 0.263 \qquad W_\gamma = \frac{C_0 - C_\alpha}{C_\gamma - C_\alpha} = \frac{0.3 - 0.02}{0.38} = 0.737$$

Point e (just above 727 °C): $C_\alpha$ = 0.02, $C_\gamma$ = 0.76 % C, length 0.74 (Slide 17 prints $C_\alpha$ = 0.02 at d and e; at f the diagram value 0.022 is used):

$$W_\alpha = \frac{0.76 - 0.3}{0.76 - 0.02} = \frac{0.46}{0.74} = 0.622 \qquad W_\gamma = \frac{0.3 - 0.02}{0.74} = 0.378$$

Point f (just below 727 °C): two microconstituents (primary α and pearlite) and two phases (α and Fe₃C):

$$W_{\alpha,\text{total}} = \frac{6.67 - 0.3}{6.67 - 0.022} = \frac{6.37}{6.648} = 0.958 \qquad W_{\alpha_p} = \frac{C_E - C_0}{C_E - C_\alpha} = \frac{0.76 - 0.3}{0.76 - 0.022} = \frac{0.46}{0.738} = 0.623$$
$$W_{\alpha_E} = W_{\alpha,\text{total}} - W_{\alpha_p} = 0.958 - 0.623 = 0.335 \qquad W_{\text{Fe}_3\text{C}} = 1 - 0.958 = 0.042 \qquad W_{\text{pearlite}} = 1 - 0.623 = 0.377$$

Checks: the primary ferrite at f equals the ferrite at e (0.62): it does not change at 727 °C. The pearlite, 0.377, equals the austenite at e (0.378; the 0.001 gap, here and in the primary ferrite 0.622/0.623, comes only from the 0.02 printed at e against 0.022 at f), and it is $0.377 \times 0.889 = 0.335$ ferrite and $0.377 \times 0.111 = 0.042$ cementite, the numbers above. The slides round these to 26/74, 62/38 and 96, 62, 34 and 4 %.

14.3 Hypereutectoid steels, $C_0$ > 0.76 % C [Session 9 Slides 19-20]

Two microconstituents: pearlite and proeutectoid cementite, $(\text{Fe}_3\text{C})_P$, which forms a network along the boundaries of the former austenite grains when the steel crosses the $A_{cm}$ line.

Cooling of a hypereutectoid steel (1.2 % C)
Figure 70. Hypereutectoid steel C1: g only γ; h, proeutectoid Fe3C at the γ grain boundaries below the Acm line; i, proeutectoid Fe3C and pearlite. Copied from Session 9 Slide 19.
Micrograph of a hypereutectoid steel
Figure 71. Hypereutectoid steel: a network of proeutectoid cementite (light) around pearlite colonies. From Session 9 Slide 19.
Microstructures of 0.4, 0.8 and 1.2 % C steels
Figure 72. Microstructures on cooling of steels with 0.4, 0.8 and 1.2 % C. The figure uses older values (0.8 % C, 723 °C). From Session 9 Slide 20.
Worked example 17 — The 1.2 % C steel of Slide 20 [Session 9 Slides 4, 19-20]

Just below 727 °C, with the values of the diagram of Slide 4 (0.022, 0.76 and 6.67 % C).

Microconstituents (short tie line from the eutectoid austenite, 0.76, to Fe₃C, 6.67; length 5.91):

$$W_{\text{Fe}_3\text{C},p} = \frac{C_0 - C_E}{C_{\text{Fe}_3\text{C}} - C_E} = \frac{1.2 - 0.76}{6.67 - 0.76} = \frac{0.44}{5.91} = 0.074 \qquad W_{\text{pearlite}} = \frac{6.67 - 1.2}{5.91} = \frac{5.47}{5.91} = 0.926$$

Phases (long tie line, 0.022 to 6.67):

$$W_{\text{Fe}_3\text{C}} = \frac{1.2 - 0.022}{6.67 - 0.022} = \frac{1.178}{6.648} = 0.177 \qquad W_\alpha = 1 - 0.177 = 0.823$$

Check: the cementite inside the pearlite is $0.926 \times 0.111 = 0.103$, and $0.074 + 0.103 = 0.177$ ✓. Answer: a thin network of proeutectoid cementite (7 %) around pearlite (93 %); even this hard steel is 82 % ferrite by mass. (The drawing of Slide 20 uses older values, 0.8 % C and 723 °C, for the eutectoid point.)

§ 15 Pearlitic transformations and cooling rate [Session 9 Slide 21]

If the cooling rate increases, the eutectoid point moves towards lower temperatures and lower carbon contents. Consequences: the percentage of proeutectoid (primary) ferrite decreases and the spacing of the pearlite lamellae decreases, which increases its hardness (fine pearlite instead of coarse pearlite).

Effect of the cooling rate on the eutectoid
Figure 73. With a higher cooling rate the eutectoid point moves to lower temperatures and lower carbon contents. From Session 9 Slide 21.
Coarse and fine pearlite
Figure 74. Coarse pearlite (slow cooling, top) and fine pearlite (fast cooling, bottom). From Session 9 Slide 21.

§ 16 Influence of the alloying elements [Session 9 Slides 22-23]

Other elements in the Fe-C system change the temperature and the composition of the eutectoid point:

Effect of Cr and Mn on the Fe-C diagram
Figure 75. α-stabilising elements such as Cr shift the eutectoid to higher temperature and lower %C; γ-stabilising elements such as Mn shift it to lower temperature and lower %C. From Session 9 Slide 22.
Eutectoid composition and temperature against alloying content
Figure 76. Influence of alloying elements on the eutectoid composition (left) and temperature (right). From Session 9 Slide 23.

In both cases the eutectoid composition falls, so a given steel lies closer to (or beyond) the eutectoid point: a hypoeutectoid steel with a γ-stabiliser such as Ni has less proeutectoid ferrite and more pearlite than the plain carbon steel of the same carbon content (used in Problem FC08).

Part IV — Phase diagrams IV: ceramic and ternary diagrams (Session 10)

§ 17 Ceramic phase diagrams [Session 10 Slides 2-4]

Ceramic systems are read with the same tools as metallic ones: the components are now compounds (oxides), and the phases can be solid solutions, intermediate compounds and the liquid.

17.1 Al₂O₃-Cr₂O₃: complete solid solubility [Session 10 Slide 2]

Al₂O₃ and Cr₂O₃ form a complete interval of solid solution, Al₂₋ₓCrₓO₃, below the solidus temperature (about 2100 °C) and down to 950 °C: the diagram has the lens shape of an isomorphous system (§4), between the melting points of Al₂O₃ (2045 ± 5 °C) and Cr₂O₃ (2275 ± 25 °C).

The Al2O3-Cr2O3 phase diagram
Figure 77. Al2O3-Cr2O3: a lens-shaped liquid + solid solution region between the melting points of Al2O3 (2045 ± 5 °C) and Cr2O3 (2275 ± 25 °C), and the solid solution Al2-xCrxO3 below it. Copied from Session 10 Slide 2.

Below 950 °C there is immiscibility: two crystalline phases, or solid solutions, exist (the dome at the bottom of the second diagram of the slide).

Al2O3-Cr2O3 down to 600 °C
Figure 78. Al₂O₃-Cr₂O₃ over a wider temperature range: complete solid solution between about 2100 and 950 °C, and two solid solutions (immiscibility) below 950 °C. From Session 10 Slide 2.

17.2 Al₂O₃-SiO₂ and mullite [Session 10 Slides 3-4]

The Al₂O₃-SiO₂ system has an intermediate phase, mullite, which includes the compound 3Al₂O₃·2SiO₂ and exists as a solid solution over a small range of compositions. The other solid phases are alumina (Al₂O₃) and cristobalite (SiO₂).

The Al2O3-SiO2 phase diagram
Figure 79. Al2O3-SiO2 with the eutectic at 1587 ± 10 °C, the mullite solid solution and the line at 1890 ± 10 °C where mullite melts incongruently. Copied from Session 10 Slide 3.
$$L\,(7.7\ \text{wt\% Al}_2\text{O}_3) \rightarrow 3\text{Al}_2\text{O}_3\cdot 2\text{SiO}_2 + \text{SiO}_2$$
$$L\,(77\ \text{wt\% Al}_2\text{O}_3) + \text{Al}_2\text{O}_3 \rightarrow 3\text{Al}_2\text{O}_3\cdot 2\text{SiO}_2$$
Temperatures of the Al₂O₃-SiO₂ diagrams

The text of Slide 3 gives 1828 °C for the peritectic, while the diagram on the same slide marks that line at 1890 ± 10 °C; the diagram of Slide 4, from another source, gives 1840 °C and about 1850 °C, and 1590 °C for the eutectic. They are different measurements of the same system; the figure above is the diagram of Slide 3. Slide 4 also writes "Al₂O₂ - SiO₂" for Al₂O₃-SiO₂.

The diagram of Slide 4 (composition in wt% SiO₂, reversed with respect to Slide 3) shows the refractories made in this system and their microstructures: alumina refractory, mullite refractory, firebrick and silica brick.

Refractories and microstructures in Al2O3-SiO2
Figure 80. Al₂O₃-SiO₂ (composition in wt% SiO₂) with the microstructures of alumina and mullite refractories, firebrick and silica brick; mullite, 3Al₂O₃·2SiO₂, is the intermediate phase. From Session 10 Slide 4.
Worked example 18 — The eutectic product of Al₂O₃-SiO₂ [Session 10 Slide 3]

Question. A liquid of eutectic composition (7.7 wt% Al₂O₃) solidifies at 1587 °C. How much mullite and how much cristobalite does the product contain?

Tie line just below 1587 °C, from cristobalite (0 wt% Al₂O₃) to mullite (ss), whose Al₂O₃-poor limit is at about 72 wt% Al₂O₃ (a reading of the figure):

$$W_{\text{mullite}} = \frac{C_0 - C_{\text{SiO}_2}}{C_{\text{mullite}} - C_{\text{SiO}_2}} = \frac{7.7 - 0}{72 - 0} = 0.107 \qquad W_{\text{SiO}_2} = \frac{72 - 7.7}{72} = \frac{64.3}{72} = 0.893$$

Check: $0.107 \times 72 + 0.893 \times 0 = 7.7$ wt% Al₂O₃. Answer: the eutectic is about 89 % cristobalite and 11 % mullite: the liquid is very rich in SiO₂, so the product is mostly silica.

§ 18 Ternary phase diagrams [Session 10 Slides 5-8]

18.1 The composition triangle [Session 10 Slide 5]

A ternary diagram has 3 components (A, B, C). The compositions are drawn in an equilateral triangle:

Composition triangle of a ternary system
Figure 81. Composition triangle of a ternary system A-B-C (A at the top, C bottom left, B bottom right) with a 10 % grid on each side. Copied from Session 10 Slide 5.

With temperature added as a vertical axis the diagram becomes a solid: the binary diagrams are its side faces, and the liquidus and solidus become surfaces.

Space model of a ternary diagram
Figure 82. A ternary phase diagram as a solid: composition in the triangle base, temperature upwards. From Session 10 Slide 5.

How to read a point. Each percentage is read along the lines parallel to the side opposite the corresponding component: the lines of constant A are parallel to the side B-C, and A grows from 0 % on that side to 100 % at the corner A. Drawing through the point the three lines parallel to the sides gives the three percentages on the three axes.

18.2 Ternary diagrams of metallic alloys [Session 10 Slides 6-7]

Because the solid has three dimensions, ternary diagrams are shown as projections or sections: the liquidus surface and the solidus surface projected onto the triangle (with their temperature contours), and isotherms, horizontal sections at one temperature. The Ag-Cu-Zn system is shown in the three ways, with an isotherm at 350 °C [Slide 6].

Ag-Cu-Zn liquidus, solidus and 350 °C isotherm
Figure 83. Ag-Cu-Zn: projections of the liquidus and solidus surfaces and the isotherm at 350 °C. From Session 10 Slide 6.

The Fe-Cr-Ni diagram (stainless steels) is shown as an isotherm at 650 °C, with the phase fields α, γ, σ and their two-phase regions [Slide 7]:

Fe-Cr-Ni isotherm at 650 °C
Figure 84. Fe-Cr-Ni isotherm at 650 °C (stainless steels) with points 1 and 2. From Session 10 Slide 7.
Worked example 19 — Reading points 1 and 2 of the Fe-Cr-Ni isotherm [Session 10 Slide 7]

Point 1. The line through the point parallel to the Fe-Ni side meets the chromium axis at 60 % Cr; the line parallel to the Cr-Ni side meets the iron axis at 20 % Fe; the line parallel to the Fe-Cr side meets the nickel axis at 20 % Ni.

Cr Fe Ni 1 60 % Cr 20 % Fe 20 % Ni
Figure 85. Reading of point 1 of the Fe-Cr-Ni isotherm at 650 °C: the three lines through it parallel to the sides meet the axes at 60 % Cr, 20 % Ni and 20 % Fe. Reading construction for point 1 of Session 10 Slide 7; the slide prints the values but does not draw these lines (EXTRA).

Check: $60 + 20 + 20 = 100$ %. At 650 °C the point lies in the field α + γ, so the alloy has two phases, as the slide says.

Point 2, the commercial stainless steel: 74 % Fe + 18 % Cr + 8 % Ni ($74 + 18 + 8 = 100$ %). It lies near the Fe corner (it is mostly iron), on the low-Ni side of the diagram.

18.3 Ceramic ternary diagrams [Session 10 Slide 8]

Ternary diagrams are also used to describe ceramics: the CaO-Al₂O₃-SiO₂ system places cements (Portland clinker, calcium aluminate cements), glasses, slags and refractories; the clay-feldspar-quartz triangle gives the composition of traditional ceramics (porcelains, pottery, earthenware), with arrows for the changes in acid resistance and porosity.

CaO-Al2O3-SiO2 and clay-feldspar-quartz diagrams
Figure 86. Ceramic ternary diagrams: CaO-Al₂O₃-SiO₂ (cements, glasses, refractories) and clay-feldspar-quartz (traditional ceramics: porcelains, pottery, earthenware). From Session 10 Slide 8.